This section describes the preparation of wood-supported polyaniline nanorods in supercapacitors (PANI/wood) using natural wood as the green matrix via a scalable and easily operable impregnation-oxidative polymerization-freeze-drying method by XUANSN. Scanning electron microscopy (SEM) revealed a large number of PANI nanorods with diameters of 31–72 nm and lengths of 240–450 nm covering the wood surface. Fourier transform infrared spectroscopy (FTIR) analysis provided further evidence for the presence of a PANI coating on the wood substrate. Furthermore, X-ray photoelectron spectroscopy (XPS) showed strong hydrogen bonds between the nitrogen atoms carrying lone pairs of electrons on the PANI and the -OH groups of the wood, which play a crucial role in interfacial bonding. This core-shell composite material can be used as a self-supporting supercapacitor electrode, exhibiting a high specific capacitance of 304 F/g at a current density of 0.1 A/g, a coulombic efficiency of 93%–100%, and a capacitance retention of 72.3% after 5000 cycles (moderate cycling stability). These experimental results demonstrate the potential of natural wood as a substrate for novel environmentally friendly energy storage devices, particularly in the application of polyaniline nanorods in supercapacitors.
1. Preparation of Wood-Supported Polyaniline Nanorods via Chemical Polymerization
This section describes the synthesis of PANI/wood composites using a scalable, simple, and efficient method comprising three steps: impregnation with an aniline monomer solution, in-situ oxidative polymerization, and freeze-drying. This method successfully prepared polyaniline nanorods in supercapacitors composites. As shown in Figure 1, cleaned natural wood was first impregnated with an aqueous solution of aniline monomer, followed by the addition of an oxidant [(NH4)2S2O8] and a dopant (HCl). Finally, the reacted wood chips were washed and freeze-dried. During impregnation, hydrogen bonding occurs between the lone pair of electrons in the nitrogen of aniline and the -OH groups of the wood matrix, resulting in complete self-assembly of the aniline monomer on the wood surface. With the addition of the oxidant, aniline undergoes in-situ oxidative polymerization. Detailed polymerization mechanisms of aniline can be found in previous literature. In this polymerization process, dried wood chips (approximately 0.75 g) were immersed in a 100 mL solution of aniline monomers at room temperature with a magnetic stirring ring for 24 hours, allowing the aniline monomers to fully self-assemble onto the wood surface via hydrogen bonding. The wood/aniline mass ratio was 1:10. After impregnation, the system was cooled to 0°C in an ice-water bath. Then, a mixture of an oxidant (ammonium persulfate, 0.08 mol) and a dopant (hydrochloric acid, 1 mol/L, 96 mL) was added dropwise to the system, and the mixture was maintained at 0–10°C for 4 hours. Finally, the wood chips were rinsed sequentially with distilled water and tert-butanol, and then freeze-dried at a pressure of 25 Pa for 24 hours to obtain the wood-supported PANI nanorod composite material. Freeze-drying is achieved by freezing the sample and then reducing the surrounding pressure to allow the frozen liquid in the sample to sublimate directly from the solid phase to the gas phase. Freeze-drying is used to maintain the morphology of polyaniline nanorods in supercapacitors before and after the drying process.

2. Microstructure of Wood-Supported Polyaniline Nanorods
The morphological characteristics of PANI before and after polymerization onto the wood surface were observed by SEM. Figure 2(a) clearly shows that the natural wood substrate is a porous material with pore sizes ranging from 3 to 7 μm. After PANI polymerization on the wood, it can be seen that the wood surface is tightly covered by a large amount of nanomaterials [Figure 2(b)], causing the wood surface color to change from light yellow to black [insets in Figures 2(a) and (b)]. According to the high-resolution SEM image (160,000×) shown in Figure 2(c), it is clear that these PANI nanorods have a diameter of 31–72 nm and a length of 140–450 nm and are randomly entangled with each other. The elemental composition of the material was analyzed by energy-dispersive X-ray (EDX) spectroscopy: As shown in Figure 2(d), in addition to the common C, O, and Au elements (derived from the SEM observation of the conductive layer), N and S elements in the polyaniline nanorods in supercapacitors composite material were also detected. The N and S elements originated from the PANI coating and residual ammonium persulfate, respectively. Furthermore, the carbon-oxygen mass ratio increased from 25 (natural wood) to 6.2 (P4N wood), indicating a large amount of PANI on the wood surface.

3.Summary
This study explores the preparation, synthesis, and characterization of wood-supported polyaniline nanorods (PANI/wood) for use in supercapacitors. The process involves a scalable, green approach using natural wood as a substrate, with a combination of impregnation, oxidative polymerization, and freeze-drying techniques. The resulting composite material, characterized by scanning electron microscopy (SEM), Fourier transform infrared spectroscopy (FTIR), and X-ray photoelectron spectroscopy (XPS), shows a significant amount of PANI nanorods (31–72 nm in diameter, 240–450 nm in length) uniformly distributed on the wood surface. The wood-supported PANI nanorods exhibit excellent electrochemical performance with a specific capacitance of 304 F/g, a high coulombic efficiency of 93%–100%, and moderate cycling stability (72.3% retention after 5000 cycles). This approach demonstrates the potential of using natural wood as an eco-friendly substrate for high-performance supercapacitor electrodes, highlighting its promising role in sustainable energy storage applications.